Thin polyester and cotton are directly pre-processed
Singeing machine, singeing and floating wool, smooth cloth surface
More than 300g rolled and cold piled for 24 hours.
Pre-treatment, boiling to remove cotton incrustations, slurry and impurities
90 degree water boiling 4 times, 100 degree steamer for 4 hours, 6 hot water tanks, 100 degree steamer, 6 water boiling, steaming to dryness, rolling cloth
Cotton imported boilable polyester and cotton
Mercerizing machine is mainly used to shape and determine the width of the fabric and increase the brightness of the cloth surface.
The gray cloth is shaped to prevent shrinkage, 3% shrinkage
The alkali tank and hot water tank washing temperatures are different.
Two-bath method, dyeing cotton first and then polyester.
Pad dyeing, dyeing, baking to develop the color of dispersed polyester, steaming to develop the color of cotton, washing to float the color, drying, tentering the finished product
Flame retardant, the dyeing agent is Bluben, the flame retardant is rolled, and the baking and ammonia fumigation allow the flame retardant to have a chemical effect, followed by full washing, drying, and stenter
Printing, baking and color fixation
Wash with evaporated water to remove floating color and dry
Add softener, dry, and set the width.
Pre-shrinking machine, fixed shrinkage rate, increased soft feel
Super soft machine, unmatched hand feel, more fluffy and soft